Injection Molding Processing Recommendations of PC/ABS Alloy

                                               
Injection Molding Unit TH1000 TH1000HF TH1200 TH1200HF TH1300 TH1300HF AM1000
drying temperature 90-100 90-100 90-100 90-100 90-100 90-100 90-100
drying time hrs 3-4h 3-4h 3-4h 3-4h 3-4h 3-4h 3-4h
maximum humidity ratio % 0.04 0.04 0.04 0.04 0.04 0.04 0.04
molding temperature  ℃  240-270 240-270 240-280 240-280 240-280 240-280 240-280
mold temperature 60-90 60-90 60-90 60-90 60-90 60-90  60-90
back pressure MPa 0.3-0.7 0.3-0.7 0.3-0.7 0.3-0.7  0.3-0.7 0.3-0.7 0.3-0.7
screw rev rpm 30-80 30-80 30-80 30-80 30-80 30-80 30-80
molding ejection volume per time % 30-80 30-80 30-80 30-80 30-80 30-80 30-80 
injection molding pressure MPa 50-160 50-160 50-160 50-160 50-160 50-160 50-160

      

Injection Molding Unit AM2000 AM3000 THF6000NH THF6100NH THF6200NH THF6300NH THF6400NH
drying temperature   100-110 100-110 80-90 80-90 80-90 90-100 90-100
drying time hrs 3-4h 3-4h 3-4h 3-4h 3-4h 3-4h 3-4h
maximum humidity ratio % 0.04 0.04 0.04 0.04 0.04 0.04 0.04
molding temperature 240-280 240-280 230-270 230-270 230-270 240-270 240-270
mold temperature 60-90 60-90 50-80 50-80 50-80 50-80 50-80
back pressure  MPa 0.3-0.7 0.3-0.7 0.3-0.7 0.3-0.7 0.3-0.7 0.3-0.7 0.3-0.7
screw rev rpm 40-70 40-70 40-70 40-70 40-70 40-70 40-70
molding ejection volume per time % 30-80 30-80 30-80 30-80 30-80 30-80 30-80
injection molding pressure MPa 50-160 50-160 50-160 50-160 50-160 50-160 50-160